文章摘要
张美娟,郄喜望,南海,等.含细长孔ZTC4/TA2钛合金铸件界面熔合效果研究[J].精密成形工程,2018,10(3):1-5.
ZHANG Mei-juan,QIE Xi-wang,NAN Hai,et al.Interfacial Fusion Effect of ZTC4/TA2 Titanium Castings with Elongated Hole[J].Journal of Netshape Forming Engineering,2018,10(3):1-5.
含细长孔ZTC4/TA2钛合金铸件界面熔合效果研究
Interfacial Fusion Effect of ZTC4/TA2 Titanium Castings with Elongated Hole
投稿时间:2018-04-24  修订日期:2018-05-10
DOI:10.3969/j.issn.1674-6457.2018.03.001
中文关键词: 钛合金  镶铸  界面  熔合率
英文关键词: titanium alloy  cast-in  interface  fusion rate
基金项目:工信部民用飞机专项科研项目(MJ-2014-G-25)
作者单位
张美娟 1. 中国航发北京航空材料研究院北京 1000952. 北京百慕航材高科技股份有限公司北京 1000943. 北京市先进钛合金精密成型工程技术研究中心北京 100095 
郄喜望 1. 北京百慕航材高科技股份有限公司北京 1000942. 北京市先进钛合金精密成型工程技术研究中心北京 100095 
南海 1. 中国航发北京航空材料研究院北京 1000952. 北京市先进钛合金精密成型工程技术研究中心北京 100095 
吴国清 北京航空航天大学北京 100083 
摘要点击次数: 4659
全文下载次数: 3522
中文摘要:
      目的 研究镶铸复合机理和钛合金镶铸件的界面熔合效果。方法 采用熔模精密铸造和镶铸技术复合的方法制备含细长孔的钛合金铸件,通过酸洗减薄管体壁厚的方式增加镶铸比,探讨镶铸比对铸件组织、界面及熔合率的影响,并分析管体被熔透的临界壁厚值。结果 铸件基体组织主要由片状的α相和残余的β晶界构成,管体是片状的魏氏体组织。铸件界面熔合率随着镶铸比增加而增大。在本实验条件下,当铸件为8︰1时,铸件熔合率超过80%;当镶铸比超过15︰1时,铸件内部管体出现熔透现象。结论 采用熔模精密铸造和镶铸技术复合的方法可制备含细长孔的钛合金铸件,并且通过减薄管体的方式可提高铸件界面熔合率。
英文摘要:
      This paper aims to research the recombination mechanism of cast in and the interfacial fusion effect of titanium alloy cast on parts. Investment casting and cast-in technology were adopted to prepare titanium alloy castings with elongated hole. An acid pickling process was introduced to slim the tube wall to increase the inlaying proportion. Effects of inlaying proportion on microstructure, interface and fusion rate were discussed along with the critical wall thickness of the melt through pipe body. The results show that, the microstructure of the matrix castings was mainly consisted of flake α and β grain boundary; and the tube body was a sheet widmanstatten structure. The interfacial fusion rate of castings went up with the increase of the inlaying proportion. When the inlaying proportion was above 8︰1, the fusion rate of the castings was more than 80%. When the inlaying proportion was above 15︰1, fusion penetration phenomenon happened in the tube body. As a conclusion, titanium alloy castings with elongated hole can be formed by investment casting and cast-in technology, and the interfacial fusion rate of castings can be increased by reducing wall thickness of the tube.
查看全文   查看/发表评论  下载PDF阅读器
关闭

关于我们 | 联系我们 | 投诉建议 | 隐私保护 | 用户协议

您是第14002567位访问者    渝ICP备15012534号-6

>版权所有:《精密成形工程》编辑部 2014 All Rights Reserved

>邮编:400039 电话:023-68679125传真:02368792396 Email: jmcxgc@163.com

>    

渝公网安备 50010702501719号